메뉴 건너뛰기




Volumn 28, Issue 3-4, 2003, Pages 431-451

Hydrogen embrittlement in power plant steels

Author keywords

Cold cracking; Control of hydrogen embrittlement; Hydrogen embrittlement; Power plant components; Steels

Indexed keywords

BOILERS; BOLTS; HYDROGEN EMBRITTLEMENT; NUTS (FASTENERS); POWER PLANTS; STEAM GENERATORS; STEAM PIPELINES; TUBES (COMPONENTS); WATER PIPELINES;

EID: 0242380229     PISSN: 02562499     EISSN: None     Source Type: Journal    
DOI: 10.1007/BF02706442     Document Type: Article
Times cited : (105)

References (50)
  • 1
    • 0019579117 scopus 로고
    • The threshold stress intensity for hydrogen-induced crack growth
    • Akhurst K N, Baker T 1981 The threshold stress intensity for hydrogen-induced crack growth. J. Metall. Trans. All: 1059-1070
    • (1981) J. Metall. Trans. All , pp. 1059-1070
    • Akhurst, K.N.1    Baker, T.2
  • 3
    • 0242284295 scopus 로고    scopus 로고
    • Variation in diffusible hydrogen content and hydrogen assisted cracking susceptibility of Cr-Mo steels
    • Albert S K, Gill T P S, Ramasubbu V, Kulkarni S D 1996 Variation in diffusible hydrogen content and hydrogen assisted cracking susceptibility of Cr-Mo steels. Intl. Weld. Conference-1996, A054: 1-8
    • (1996) Intl. Weld. Conference-1996 , vol.A054 , pp. 1-8
    • Albert, S.K.1    Gill, T.P.S.2    Ramasubbu, V.3    Kulkarni, S.D.4
  • 5
    • 0242379012 scopus 로고
    • Failure of high pressure steam pipe
    • (ed.) Khlefa A Easaklul (Materials Park, OH: ASM Int.)
    • Antonio C D 1993 Failure of high pressure steam pipe. Handbook of case histories in failure analysis (ed.) Khlefa A Easaklul (Materials Park, OH: ASM Int.) vol.2, 181-184
    • (1993) Handbook of Case Histories in Failure Analysis , vol.2 , pp. 181-184
    • Antonio, C.D.1
  • 7
    • 0015300738 scopus 로고
    • A new model for hydrogen assisted cracking (hydrogen embrittlement)
    • Beachem C D 1972 A new model for hydrogen assisted cracking (hydrogen embrittlement). Metall. Trans. A3: 437-451
    • (1972) Metall. Trans. A , vol.3 , pp. 437-451
    • Beachem, C.D.1
  • 8
    • 0024657268 scopus 로고
    • Influence of nitrogen ion implantation on hydrogen permeation in an extra mild steel
    • Brass A M, Chene J, Pivin J C 1989 Influence of nitrogen ion implantation on hydrogen permeation in an extra mild steel. J. Mater. Sci. 24: 1693-1700
    • (1989) J. Mater. Sci. , vol.24 , pp. 1693-1700
    • Brass, A.M.1    Chene, J.2    Pivin, J.C.3
  • 10
    • 0242379006 scopus 로고
    • Environmentally induced fracture of type 410 martensitic stainless steel self-drilling tapping screws
    • (ed.) Khlefa A Esaklul, (Materials Park, OH: ASM Int.)
    • Chakrapani D G 1993 Environmentally induced fracture of type 410 martensitic stainless steel self-drilling tapping screws. Handbook of case histories in failure analysis, (ed.) Khlefa A Esaklul, (Materials Park, OH: ASM Int.) vol.1, 305-307
    • (1993) Handbook of Case Histories in Failure Analysis , vol.1 , pp. 305-307
    • Chakrapani, D.G.1
  • 11
    • 0242284293 scopus 로고
    • Influence of bulk and grain boundary phosphorus content on hydrogen induced cracking in low strength steels
    • Dayal R K, Grabke H J 1987 Influence of bulk and grain boundary phosphorus content on hydrogen induced cracking in low strength steels. Steel Res. 58: 179-185
    • (1987) Steel Res. , vol.58 , pp. 179-185
    • Dayal, R.K.1    Grabke, H.J.2
  • 12
    • 0023387434 scopus 로고
    • Hydrogen stress corrosion cracking in low and high strength ferritic steels of different phosphorus content in acidic media
    • Dayal R K, Grabke H J 1987 Hydrogen stress corrosion cracking in low and high strength ferritic steels of different phosphorus content in acidic media. Werkstoffe Korrosion 38: 409-4-16
    • (1987) Werkstoffe Korrosion , vol.38 , pp. 409-416
    • Dayal, R.K.1    Grabke, H.J.2
  • 13
    • 0029180363 scopus 로고
    • Hydrogen-induced cracking of low carbon-low alloy steel weldments
    • Davidson J E 1995 Hydrogen-induced cracking of low carbon-low alloy steel weldments. Mater. Forum 19: 35-51
    • (1995) Mater. Forum , vol.19 , pp. 35-51
    • Davidson, J.E.1
  • 15
    • 0024620514 scopus 로고
    • Protection against hydrogen embrittlement by ion beam mixing
    • Ensinger W, Wolf G K 1989 Protection against hydrogen embrittlement by ion beam mixing. Nucl. Instrum. Methods B39: 552-555
    • (1989) Nucl. Instrum. Methods B , vol.39 , pp. 552-555
    • Ensinger, W.1    Wolf, G.K.2
  • 16
    • 0017517018 scopus 로고
    • Gaseous hydrogen embrittlement of high strength steels
    • Gangloff R P, Wei R P 1977 Gaseous hydrogen embrittlement of high strength steels. Metall. Trans. A8: 1043-1053
    • (1977) Metall. Trans. A , vol.8 , pp. 1043-1053
    • Gangloff, R.P.1    Wei, R.P.2
  • 18
    • 0242379002 scopus 로고
    • Hydrogen damage of waterwall tubes
    • (ed.) Khlefa A Easaklul (Materials Park, OH: ASM Int.)
    • Hahn S J 1993 Hydrogen damage of waterwall tubes. Handbook of case histories in failure analysis (ed.) Khlefa A Easaklul (Materials Park, OH: ASM Int.) vol.2, 490-492
    • (1993) Handbook of Case Histories in Failure Analysis , vol.2 , pp. 490-492
    • Hahn, S.J.1
  • 19
    • 0242347457 scopus 로고
    • An unusual case of hydrogen induced failure in a refinery boiler tube
    • (ed.) Khlefa A Easaklul (Materials Park, OH: ASM Int.)
    • Islam M 1993 An unusual case of hydrogen induced failure in a refinery boiler tube. Handbook of case histories in failure analysis (ed.) Khlefa A Easaklul (Materials Park, OH: ASM Int.) vol. 2, 145-147
    • (1993) Handbook of Case Histories in Failure Analysis , vol.2 , pp. 145-147
    • Islam, M.1
  • 20
    • 0242284294 scopus 로고
    • Hydrogen induced cracking of welded truss gusset plates
    • (ed.) Khlefa A Easaklul (Materials Park, OH: ASM Int.)
    • Jones W F 1993 Hydrogen induced cracking of welded truss gusset plates. Handbook of case histories in failure analysis (ed.) Khlefa A Easaklul (Materials Park, OH: ASM Int.) vol. 1, 382-384
    • (1993) Handbook of Case Histories in Failure Analysis , vol.1 , pp. 382-384
    • Jones, W.F.1
  • 21
    • 0015361108 scopus 로고
    • Slow crack growth in hydrogen & hydrogen sulphide gas environment
    • Kerns G E, Staehle R W 1972 Slow crack growth in hydrogen & hydrogen sulphide gas environment. Scr. Metall. 6:631-634
    • (1972) Scr. Metall. , vol.6 , pp. 631-634
    • Kerns, G.E.1    Staehle, R.W.2
  • 22
    • 0025475655 scopus 로고
    • Hydrogen assisted ductile fracture in spheroidised steel
    • Kwon DI, Asaro R J 1990 Hydrogen assisted ductile fracture in spheroidised steel. Acta Metall. Mater. 38: 1595-1606
    • (1990) Acta Metall. Mater. , vol.38 , pp. 1595-1606
    • Kwon, D.I.1    Asaro, R.J.2
  • 23
    • 0003053955 scopus 로고
    • Effect of hydrogen on the mechanical properties of low carbon and austenitic steels
    • (eds) I M Bernstein, A W Thompson (Metals Park, OH: ASM Int.)
    • Louthan M R 1974 Effect of hydrogen on the mechanical properties of low carbon and austenitic steels. Hydrogen in metals (eds) I M Bernstein, A W Thompson (Metals Park, OH: ASM Int.) p. 53
    • (1974) Hydrogen in Metals , pp. 53
    • Louthan, M.R.1
  • 24
    • 2742591835 scopus 로고
    • Dissertation, ETH No. 8432, Swiss Federal Institute of Technology, Zurich
    • Magdowski 1987 SCCoflow alloy steels in water, Dissertation, ETH No. 8432, Swiss Federal Institute of Technology, Zurich
    • (1987) SCCoflow Alloy Steels in Water
    • Magdowski1
  • 25
  • 26
    • 0018453541 scopus 로고
    • The effects of segregated impurities on intergranular fracture energy
    • McMahon C J Jr, Vitek V 1979 The effects of segregated impurities on intergranular fracture energy. Acta Metall. 27:507-513
    • (1979) Acta Metall. , vol.27 , pp. 507-513
    • McMahon Jr., C.J.1    Vitek, V.2
  • 27
    • 55449132005 scopus 로고    scopus 로고
    • Corrosion 9th edn. (Metals Park, Ohio: ASM int.)
    • Metals handbook 1987 vol.13, Corrosion 9th edn. (Metals Park, Ohio: ASM int.)
    • Metals Handbook 1987 , vol.13
  • 29
    • 0025225786 scopus 로고
    • Hydrogen effects on the properties and fracture modes of iron based alloys
    • Moody N R, Robinson S L 1990 Hydrogen effects on the properties and fracture modes of iron based alloys. Res Mech. 30: 143-206
    • (1990) Res Mech. , vol.30 , pp. 143-206
    • Moody, N.R.1    Robinson, S.L.2
  • 30
    • 55449138224 scopus 로고    scopus 로고
    • Hydrogen damage of metallic materials and its prevention, ATM 99
    • Namboodhiri T K G 1999 Hydrogen damage of metallic materials and its prevention, ATM 99, Indian Inst. Technol., Kanpur, 163-180
    • (1999) Indian Inst. Technol., Kanpur , pp. 163-180
    • Namboodhiri, T.K.G.1
  • 32
    • 0007672336 scopus 로고
    • Hydrogen in metals
    • (eds) R W Staehle, A J Forty, D Van Roogen (NACE)
    • Oriani R A 1967 Hydrogen in metals Proc. Conf. Fundamental Aspects ofSCC, (eds) R W Staehle, A J Forty, D Van Roogen (NACE) 32-50
    • (1967) Proc. Conf. Fundamental Aspects OfSCC , pp. 32-50
    • Oriani, R.A.1
  • 33
    • 0016104163 scopus 로고
    • Equilibrium aspects of hydrogen induced cracking of steels
    • Oriani R A, Josephic P H 1974 Equilibrium aspects of hydrogen induced cracking of steels. Acta Metall. 22: 1065-1074
    • (1974) Acta Metall. , vol.22 , pp. 1065-1074
    • Oriani, R.A.1    Josephic, P.H.2
  • 34
    • 0242347462 scopus 로고
    • Characterisation of 9%Cr-1%Mo ferritic steel weldment for susceptibility to corrosion during hydrogen charging and repair welding
    • Parvathavarthini N, Dayal R K, Gill T P S 1995 Characterisation of 9%Cr-1%Mo ferritic steel weldment for susceptibility to corrosion during hydrogen charging and repair welding. Indian Welding J. 28 (3 & 4): 9-21
    • (1995) Indian Welding J. , vol.28 , Issue.3-4 , pp. 9-21
    • Parvathavarthini, N.1    Dayal, R.K.2    Gill, T.P.S.3
  • 36
    • 0032794983 scopus 로고    scopus 로고
    • Influence of microstructure on the hydrogen permeability of 9Cr-1Mo ferritic steels
    • Parvathavarthini N, Saroja S, Dayal R K, 1999 Influence of microstructure on the hydrogen permeability of 9Cr-1Mo ferritic steels. J. Nucl. Mater. 264: 35-47
    • (1999) J. Nucl. Mater. , vol.264 , pp. 35-47
    • Parvathavarthini, N.1    Saroja, S.2    Dayal, R.K.3
  • 38
    • 0343820034 scopus 로고    scopus 로고
    • The effect of hydrogen on dislocation dynamics
    • Robertson I M 1999 The effect of hydrogen on dislocation dynamics. Eng. Fract. Mech. 64: 649-673
    • (1999) Eng. Fract. Mech. , vol.64 , pp. 649-673
    • Robertson, I.M.1
  • 39
    • 0026875960 scopus 로고
    • Effect of hydrogen and carbon on thermally activated deformation in nickel
    • Sirois E, Birnbaum H K 1992 Effect of hydrogen and carbon on thermally activated deformation in nickel. Acta Metall. Mater. 40: 1377-1385
    • (1992) Acta Metall. Mater. , vol.40 , pp. 1377-1385
    • Sirois, E.1    Birnbaum, H.K.2
  • 42
    • 0032172981 scopus 로고    scopus 로고
    • Failure of steels caused by hydrogen induced microcracking
    • Strnadel B 1998 Failure of steels caused by hydrogen induced microcracking. Eng. Fracture Mech. 61:299-310
    • (1998) Eng. Fracture Mech. , vol.61 , pp. 299-310
    • Strnadel, B.1
  • 43
    • 0242379009 scopus 로고
    • Hydrogen embrittlement failure of steel head cap screws
    • (éd.) Khlefa A Easaklul (Materials Park, OH: ASM Int.)
    • Tanner G M 1993 Hydrogen embrittlement failure of steel head cap screws. Handbook of case histories in failure analysis (éd.) Khlefa A Easaklul (Materials Park, OH: ASM Int.) vol.1, 332-334
    • (1993) Handbook of Case Histories in Failure Analysis , vol.1 , pp. 332-334
    • Tanner, G.M.1
  • 46
    • 0003128433 scopus 로고
    • The role of metallurgical variable in hydrogen assisted environmental fracture
    • (eds) M G Fontanna, R W Staehle (New York: Plenum) vol.
    • Thompson A W, Bernstein I M 1980 The role of metallurgical variable in hydrogen assisted environmental fracture, Advances in corrosion science and technology (eds) M G Fontanna, R W Staehle (New York: Plenum) vol.7, 53-173
    • (1980) Advances in Corrosion Science and Technology , vol.7 , pp. 53-173
    • Thompson, A.W.1    Bernstein, I.M.2
  • 48
    • 84974999847 scopus 로고
    • Hydrogen assisted cracking in C-Mn and low alloy steel weldments
    • Yurioka N, Sazuki H 1990 Hydrogen assisted cracking in C-Mn and low alloy steel weldments. Int. Mater. Rev. 35: 217-249
    • (1990) Int. Mater. Rev. , vol.35 , pp. 217-249
    • Yurioka, N.1    Sazuki, H.2
  • 50
    • 0006938317 scopus 로고
    • Hydrogen embrittlement, internal stress and defects in steels
    • Zappfe C, Sims C 1941 Hydrogen embrittlement, internal stress and defects in steels. Trans. AIME 145: 225-227
    • (1941) Trans. AIME , vol.145 , pp. 225-227
    • Zappfe, C.1    Sims, C.2